Introduction
Cast metal restorations are made by the lost-wax technique: the finished wax pattern is fitted with a sprue, surrounded by a heat-resistant investment, the wax is burnt out, and molten alloy is forced into the empty mould. The topic then covers soldering and welding, the two ways of joining separately made metal parts.
Preparing the wax pattern for investing (spruing)
- Sprue former: wax, plastic or metal (hollow metal sprues are removed before burnout). It is attached to the thickest part of the pattern, away from the margins and the occlusal contacts, at about 45° to the surface, so the alloy flows in without turbulence.
- Sprue diameter is about equal to or larger than the thickest part of the pattern, so that the sprue freezes last. A reservoir (a ball of wax on the sprue close to the pattern) keeps feeding the pattern while the alloy shrinks on solidifying. This prevents localised shrinkage porosity (suck-back).
- Bridges and multi-unit work: indirect spruing with a runner bar (a horizontal bar that also serves as reservoir) and a short sprue to each unit.
- Crucible former (base): the pattern sits about 6 mm from the open end of the ring. This leaves enough investment for strength but still lets gases escape, and keeps the pattern out of the heat centre of the ring.
- Casting ring and liner: the liner is cellulose or ceramic-fibre paper (asbestos is no longer used). It lets the investment expand and stops short of the ring ends.
- The pattern is cleaned and coated with a wetting agent (surface-tension reducer) so that the investment wets it without air bubbles.