Introduction
Metal-free bridges are fixed dental prostheses whose framework is made of ceramic (mainly lithium disilicate and zirconia) or of polymers and fibre-reinforced composite, produced largely by CAD/CAM. They are chosen for aesthetics, biocompatibility, metal allergy and a digital workflow, but within stricter limits of span and connector size than metal-ceramic bridges.
Classification of metal-free materials
The Gracis classification groups ceramics by their structure:
- glass-matrix ceramics: feldspathic, leucite-reinforced, lithium disilicate
- polycrystalline ceramics: alumina, zirconia
- resin-matrix ceramics: polymer-infiltrated ceramic network, resin nano-ceramic
An older generation, glass-infiltrated alumina or zirconia (In-Ceram), is now of historic interest for bridges. The polymers are fibre-reinforced composite (FRC, with glass fibres), high-performance polymers (PEEK) and PMMA (long-term provisional use only).
Properties and indications of each material for bridges
- Lithium disilicate: a glass-ceramic, heat-pressed (lost-wax) or CAD/CAM milled in the partly crystallized lithium metasilicate ("blue") state and then fired to crystallize. Flexural strength is roughly 350–500 MPa. Aesthetics are good and it is etchable. The manufacturer indication is a 3-unit bridge in the anterior and premolar region, with the second premolar as the most distal abutment.
- Zirconia (3Y-TZP): flexural strength roughly 900–1,200 MPa. Transformation toughening (tetragonal to monoclinic with a volume increase) stops crack growth. It is opaque, so classically veneered, and is indicated for posterior and multi-unit bridges. The risk is low-temperature degradation (ageing).
- High-translucency zirconia (4Y/5Y, with a cubic phase, multilayer): better aesthetics but lower strength and toughness, and the cubic phase has no transformation toughening. Spans are limited by the manufacturers.
- Monolithic versus veneered zirconia: chipping of the veneering ceramic is the main technical problem of veneered zirconia. Monolithic (polished) zirconia avoids chipping and needs less reduction.
- FRC bridges: made chairside or in the laboratory; minimally invasive and repairable; an interim or medium-term solution.
- PEEK frameworks: biocompatible with a low modulus, but they need composite veneering and have limited long-term evidence.
- Resin-bonded all-ceramic cantilever bridges (single-retainer zirconia or lithium disilicate) for missing incisors showed high long-term survival in Kern's work. Their detail belongs to topic 10.