Introduction
Casting means melting an alloy and forcing it into a refractory mould formed around a wax pattern. Dentistry uses the lost-wax technique, introduced to dentistry by Taggart in 1907, for inlays, onlays, crowns, bridge frameworks, metal–ceramic copings and partial-denture frameworks. This topic covers melting the alloy, the force that fills the mould, the casting machines and the handling of the casting afterwards.
The lost-wax process: overview and requirements
Sequence: wax pattern, sprue, investing, burnout (wax elimination), melting, casting, cooling, divesting, cleaning (pickling or blasting), finishing. Spruing and investing are the subject of the next topic.
- A good casting has an accurate fit, complete margins, a smooth surface, no porosity and preserved alloy properties.
- Casting shrinkage of gold alloys is about 1.25–1.65%. It happens in three stages: liquid contraction (fed from the button), contraction on solidification, and thermal contraction of the solid to room temperature. Investment expansion compensates for it.
- Why force is needed: the surface tension of the molten alloy and the air in the mould (back pressure) stop gravity alone from filling a fine mould.